Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of RADILON D 40EP25ZW 7037 BL - PA610 - RadiciGroup High Performance Polymers

Material Data Center offers the following functions for RADILON D 40EP25ZW 7037 BL:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Radilon D datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
PA610 flexible, high viscosity extrusion grade. Toughened and plasticized. Heat stabilized. Blue colour.

Suitable for extrusion of pipes, profiles and cable jackets. Good impact resistance also at low temperatures. This grade is partially renewably-sourced (64% of base polymer by weight).
Processing/Physical Characteristicsdry / condUnitTest Standard
ISO Data
Molding shrinkage, parallel 1.6 / * % ISO 294-4, 2577
Molding shrinkage, normal 1.6 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
ISO Data
Tensile Modulus 550 / 380 MPa ISO 527
Stress at 50% strain 28 / 24 MPa ISO 527
Strain at break >50 / >50 % ISO 527
Charpy notched impact strength, +23°C 110 / 120 kJ/m² ISO 179/1eA
Charpy notched impact strength, -30°C 55 / - kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
ISO Data
Melting temperature, 10°C/min 218 / * °C ISO 11357-1/-3
Temp. of deflection under load, 1.80 MPa 50 / * °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 100 / * °C ISO 75-1/-2
Electrical propertiesdry / condUnitTest Standard
ISO Data
Volume resistivity 1E13 / 1E11 Ohm*m IEC 62631-3-1
Surface resistivity * / 1E10 Ohm IEC 62631-3-2
Other propertiesdry / condUnitTest Standard
Water absorption 2 / * % Sim. to ISO 62
Humidity absorption 0.9 / * % Sim. to ISO 62
Density 1050 / - kg/m³ ISO 1183
Biobased content 60 % -
Processing Recommendation Injection MoldingValueUnitTest Standard
Pre-drying - Temperature 80 °C -
Pre-drying - Time 2 - 4 h -
Processing humidity ≤0.1 % -
Melt temperature 230 - 260 °C -
Mold temperature 70 - 80 °C -
Diagrams
Stress-strain , RADILON D 40EP25ZW 7037 BL (dry), PA610, RadiciGroup
Secant modulus-strain , RADILON D 40EP25ZW 7037 BL (dry), PA610, RadiciGroup
Characteristics
Processing
Injection Molding, Pipe/Tube Extrusion, Profile Extrusion, Wire/Cable Extrusion
Delivery form
Granules
Additives
Plasticizer
Special Characteristics
High impact or impact modified, Heat stabilized or stable to heat
Certifications
Contains renewable resources
Regional Availability
Other text information
Injection molding
The material is delivered in moisture-proof packaging ready for processing. Maximum recommended water content for best processing is 0.10%. Typical conditions with a desiccant drier: temperature 80 ° C, dew point -20 ° C or below, time 2-4 h or more. Special care must be taken to avoid moisture absorption and contamination with other polymers when adding regrind material. Colour variation and mechanical properties reduction may occur and should always be carefully monitored.

Injection Molding Processing Parameters
Melt Temperature Mold Temperature Injection Speed
230 - 260°C 70 - 80°C medium
Extrusion Temperature
240 - 290°C
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.